20210430 photolitho
From mn.fysikk.laglivlab
Revision as of 12:30, 30 April 2021 by Dagkd@uio.no (talk | contribs)
- Started LAF-bench
- N2 valve had been left open, almost no pressure left!
- cleaned wafers with plasma only
- 1st wafer
- 3700 RPM ~ 20 um
- prebake on programmable hot plate
- Masking with UV-Kub 2. UV at 11% intensity for 30 sec.
- Hot plate too hot, 65C postbake happened at 72-66C
- The hot plate seems to take longer than the timer on my telephone. This needs to be checked!
- 2nd wafer 3100 RPM ~ 25 um
- prebake on VWR hot plate, no nice control of ramp in temp
- Masking with UV-Kub 2. UV at 11% intensity for 30 sec.
- Postbake on VWR hotplate