  • cleaned wafers with plasma oDag's patterns
    • 1700 RPM (1700 programmed) ~ 50 um, 1h rest
    • prebake on VWR hot plate
    • Masking with UV-Kub 2. UV at X% intensity for 30 sec.
    • > 10 minutes rest
    • post bake on VWR plate
    • > 10 minutes rest
    • Developed X min in PGMEA,
    • 2h hard bake at 135C
  • 2nd wafer
    • 900 RPM (970 in program) ~ 100 um, 1h rest
    • prebake on VWR hot plate
    • Masking with UV-Kub 2. UV at X% intensity for 30 sec.
    • >10 minutes rest
    • Postbake on VWR hotplate
    • X minutes rest
    • Developed X min in PGMEA.