PDMS

We made a new batch of PDMS. We made another one of Thomas' 25 um chip and then the whole 50 um wafer.

- Used 50g of PDMS and 5g of curing agent. This was too much PDMS, can probably use 40g PDMS and 4g curing agent next time.

The chip from Monday (05.07.2021) that we soaked in hexane collapsed after we plasma treated it and placed it on the glass. The chip was a little wonky so it may be that the design itself was a little wonky as well. For next time we will try soaking the chips in hexane, then ethanol and then water to manage the deswelling in a more controlled manner by soaking the chips in decreasingly soluble solutions.

Collagen

We made a new batch of collagen to coat one of the chips after plasma cleaning it.